Eastman Tritan Copolyester Drying and Extrusion Processing Guide

Eastman Tritan™ copolyester provides customers excellent toughness as well as clarity, chemical resistance, dimensional stability, low and stable shrinkage rates, and other enhanced physical properties. Versions of Tritan are also available with various additive packages, such as UV and color. To optimize these physical properties and widen the processing window, some drying and processing guidelines are listed.


Eastman Tritan Copolyester Drying and Extrusion Processing Guide - cover page
Brand
EASTMAN
Category
Other
Document type
User Manual
Language
English
Pages
8
File format
PDF
File size
558 KB
Published
18 November, 2023
Updated
18 November, 2023
MD5 checksum
8D968D558F693E31EDCCD9424878146E

About this manual

Eastman Tritan copolyester offers excellent toughness, clarity, chemical resistance, and dimensional stability. This document outlines specific drying and processing guidelines to optimize these properties and widen the processing window. It covers drying parameters, moisture content targets, and equipment setup requirements.

What's inside

  • Drying Guidelines
  • Extrusion Main Extruder
  • Die Setup
  • Extrusion Conditions
  • Recycling and Regrind
  • Downstream Equipment
  • Roll Stack Operation
  • Purging and Shutdown

Specifications

Target pellet moisture0.01% to 0.02% (100–200 ppm)
Dryer capacity minimum8,000 lb for 1,000 lb/hr production
Minimum airflow1 CFM per lb/hr extrusion rate
Minimum dew point temperature220°F (pref. 240°F)
Screw L/D ratio32:1
Typical screw speed100 rpm
Typical melt pump speed60 rpm
Melt temp. max.450°F (280°C)
Maximum regrind level25%

Frequently asked questions

What is the recommended drying temperature and time for Tritan?

Dry Tritan at 180°F for 6–8 hours using a desiccant dryer.

What is the ideal moisture content for Tritan pellets?

The moisture content should ideally be less than 100 ppm, though up to 200 ppm may yield acceptable quality.

What is the maximum recommended drying time?

Do not dry over 20 hours to prevent excessive molecular weight loss and property decrease.

What is the maximum melt temperature for Tritan extrusion?

The maximum melt temperature is 450°F (280°C).