Technical data sheet for PMS1112ES electrostripping salts, including preparation, equipment, process parameters and safety notes.
The PMS1112ES data sheet from Precious Metal Services provides detailed instructions for electrostripping gold and silver jewellery. It outlines solution preparation, recommended equipment, and step‑by‑step stripping procedures.
Additional notes cover cleaning, cyanide maintenance, waste disposal, and a disclaimer regarding safety and liability.
| Solution volume | 1000 ml |
|---|---|
| Gold Electro Strip salts | 50 g |
| Silver Electro Strip salts | 50 g |
| Operating temperature | approximately 60 °C |
| Voltage range | 15‑25 V |
| Current density | 50‑150 A |
Heat the solution to approximately 60 °C.
Set the voltage between 15 and 25 V.
Add 30‑50 g of potassium cyanide after 4‑6 weeks as the cyanide content declines.